Guides / Quality
Injection molding defects: causes and fixes for the 14 most common problems
October 28, 2026
Injection molding defects fall into a small set of patterns, and nearly all of them have a cause in one of four places: the part design, the mold, the process or the material. Fixing them in that order, design first and process last, gives lasting results. Fixing them the other way round leaves a fragile process that drifts every time the weather, the resin lot or the operator changes. This chart covers 14 defects, what each looks like and where to look first.
The four places a defect comes from
- Part design: wall thickness, ribs, bosses, corners, draft, flow length.
- Mold: gate location and size, venting, cooling, parting line fit, surface finish, ejection.
- Process: melt and mold temperature, injection speed and pressure, hold time, cooling time, screw speed.
- Material: wrong grade, moisture, contamination, regrind, color masterbatch.
Process changes are quick and free, so plants try them first. They also hide the root cause. A design or mold fix costs more but removes the defect. Ask the plant which category the cause belongs to and what evidence it has.
Defect chart
| Defect | What it looks like | Most likely root cause |
|---|---|---|
| Short shot | Part incomplete, cavity not filled | Mold (venting, gate), process (low pressure or temperature), design (thin walls, long flow) |
| Flash | Thin film of plastic at the parting line or around pins | Mold (worn parting line), process (high pressure), insufficient clamp force |
| Sink marks | Dents on the surface over thick sections or ribs | Design (thick sections), process (low hold pressure or time) |
| Voids | Bubbles inside thick sections | Design (thick walls), process (hold), moisture |
| Warpage | Part twists or bows after ejection | Design (uneven walls), mold (cooling), process (cooling time) |
| Weld lines | Visible or weak line where flow fronts meet | Design and gate position, process (low melt temperature) |
| Flow lines | Wavy marks near the gate or along flow | Process (low melt or mold temperature, slow fill), thin walls |
| Burn marks | Black or brown marks, often at end of fill | Mold (trapped air, poor venting), process (high speed) |
| Splay | Silver streaks, usually trailing from gate | Material (moisture), process (high melt temperature) |
| Jetting | Snake-like pattern near the gate | Mold (gate type and size), process (high speed) |
| Delamination | Surface layers peel off | Material (contamination, mixed resins), moisture |
| Black specks | Dark particles in the part | Material (contamination), process (degraded resin in barrel) |
| Ejector pin marks | Marks or stress whitening at pin locations | Mold (pin size and position), process (short cooling), design (low draft) |
| Drag marks | Scratches along the side walls | Design (low draft), mold (surface), process |
Short shot
What it looks like: a part with missing corners, thin features or ends. Design: thin walls over long flow paths, sudden section changes. Mold: blocked vents, small gates, cold slug wells missing, a restricted runner. Process: low injection pressure or speed, cold melt, low mold temperature, shot size too small. Material: resin with too high viscosity for the part. Fix order: thicken or shorten the flow path, add vents or enlarge the gate, then raise pressure, melt temperature or speed. Details in short shot in injection molding.
Flash
What it looks like: a thin fin of plastic at the parting line, at ejector pins or on slides. Design: features located on the parting line, thin steel sections that flex. Mold: worn or damaged parting line, poor fit, insufficient support, vents cut too deep. Process: injection or hold pressure too high, clamp force too low, viscosity too low from high melt temperature. Fix order: repair or re-fit the mold, then check clamp force and pack pressure. See flash in injection molding.
Sink marks and voids
What they look like: shallow dents on the surface above a thick section, rib or boss. Voids are the same effect inside the part, when the skin holds and the core pulls away. Design: rib thickness above about 50 to 60 percent of the wall, thick bosses, sudden thickness changes. Mold: gate too small or too far, so pressure does not reach the thick area before the gate freezes. Poor cooling at the thick section. Process: hold pressure or time too low, melt too hot. Fix order: thin the section or core it out, move or enlarge the gate, then extend hold time. Textured surfaces hide mild sink. See sink marks in injection molding.
Warpage
What it looks like: a flat part bows, a frame twists or box walls pull in. Design: uneven wall thickness, large flat areas, unsymmetrical ribs. Mold: uneven cooling between core and cavity, gate position that causes differential shrinkage. Process: short cooling time, high ejection temperature, too much pack in one area. Material: semi-crystalline resins (PP, PA, POM) shrink more and warp more than amorphous ones. Glass fiber adds orientation effects. Fix order: even out the walls, balance cooling, adjust gating, then lengthen cooling time or use a cooling fixture. See warpage in injection molding.
Weld lines
What they look like: a thin line where two flow fronts meet, often behind holes or posts. Weaker than the surrounding material and sometimes visible. Design: holes and bosses split the flow. Thin walls cool the fronts before they bond. Mold: gate position decides where the lines fall. Poor venting traps air at the weld. Process: low melt or mold temperature, low injection speed. Fix order: move the gate or change the design so the line lands in a low-stress, hidden area, then raise melt and mold temperature. See weld lines in injection molding.
Need a quote for a molded part? Get matched with a molding plant
Flow lines, jetting and burn marks
Flow lines are wavy marks that follow the flow. Raise melt and mold temperature, increase injection speed and use a gate that fills the cavity more evenly.
Jetting looks like a snake, where plastic shoots into the cavity without touching the walls. It means the gate is too small or sends melt straight into open space. Enlarge the gate, point it at a wall or a pin, or slow the first part of the fill.
Burn marks are dark marks at the end of the fill, where trapped air is compressed and heated. Add or clean vents, reduce speed at the end of fill and check that the vent depth suits the resin.
Splay, delamination and black specks
These three are mostly material defects.
Splay shows as silver streaks. The most common cause is moisture in hygroscopic resins such as PA, PC, PET, ABS and PBT. Dry to the supplier’s specification and check the dryer’s dew point. Overheated melt and long residence time can also cause splay. See splay in injection molding and resin drying temperature chart.
Delamination shows as peeling layers. Typical causes are moisture and mixed or contaminated resin, for example PP with a trace of another polymer.
Black specks come from degraded resin in the barrel, from contamination in regrind or from a worn screw or check ring. Purge the barrel, review regrind control and check the shot size against barrel capacity.
Ejector pin marks and drag marks
Ejector pin marks are circles or whitened areas where pins push the part. Causes include a part still too hot or soft, pins too small, pins placed on thin or visible areas and not enough draft. Fix with larger pins or sleeves, better location, longer cooling or more draft. See ejector pin marks.
Drag marks are scratches along walls in the ejection direction. The usual cause is too little draft, a rough or damaged surface, or texture without enough extra draft. See draft angle in injection molding.
How to work with a plant on a defect
A defect report that says “bad parts” gets nowhere. Ask for, or send, this:
- Photos of good and bad parts, with a scale, and close-ups of the defect.
- Frequency: shots per hour, per cavity, per lot.
- When it began: from the start, after a mold change, after a resin lot change.
- Process record: the approved setup sheet and the current settings.
- Material record: lot numbers, drying records, regrind percentage.
- Process change log: what the plant changed to try to fix it.
- Root cause analysis in the form of an 8D or similar. See 8D report for molded parts quality claims.
Agree acceptance criteria early: what size of flash, what depth of sink and what color difference are acceptable, and from which distance. Limit samples for cosmetic defects shows how.
Prevention beats correction
Most defects are cheaper to prevent in the design stage. Run a design review with the plant before steel is cut, and consider a mold flow analysis for complex parts. See mold flow analysis. The plant sees fill, weld lines and air traps before they cost money.
We are a manufacturers’ representative for audited plastic injection molding plants. If you have a part and want it matched to a plant whose lane fits, send an RFQ. It is free for buyers: the plant pays us a commission on orders from buyers we introduce, and you order from the plant directly.
Frequently asked questions
Which injection molding defect is most common?
Sink marks, warpage, flash and short shots appear most often in production, in roughly that order of frequency depending on the part. Thick sections cause sink and warp; worn or poorly fitted mold surfaces cause flash; low fill pressure or blocked vents cause short shots. Part design decides how easy they are to prevent.
Who is responsible when parts have defects, the buyer or the plant?
It depends on the cause and on what the purchase order and approved sample say. If the plant ran outside the approved process, it is the plant's issue. If the part design or the approved mold made the defect unavoidable, the fix may need a design or tool change. Agree defect limits and a corrective action process before production.
Can a defect be fixed without changing the mold?
Often, yes. Many defects respond to process changes in temperature, pressure, speed or hold time, or to better drying. But if the cause is in the part design or the mold, such as thick ribs, poor venting or bad gate location, process changes only reduce it. A lasting fix then needs a design or tool change.
Need a quote for a molded part?
Send the model. We match it to the partner plant whose lane fits and reply within 24 business hours. Free for buyers.