Short shots in injection molding: causes, fixes and what to ask the plant

November 10, 2026

A short shot is a molded part that is not complete because the melt froze or ran out before the cavity filled. You see it as a missing corner, a rib that stops short, a thin wall with a ragged edge or a part that weighs less than the others in the same lot. The cause sits in one of four places: the part design, the mold, the process or the material. Check them in that order, because the first two cost the most to fix and the last two are the quickest to try.

What a short shot looks like

Look at where the part is incomplete. The location points to the cause.

  • Far end of the flow path: the melt cooled or ran out of pressure before it got there. This is the classic short shot.
  • A thin rib or boss on a thick wall: the melt took the easy path through the thick wall and the thin feature froze before it filled.
  • One cavity of a multi-cavity mold only: an unbalanced runner, a clogged hot runner nozzle or a blocked vent in that cavity.
  • Edge with a burnt or shiny surface: air could not escape. The melt is compressing the air and stops against it.
  • Random, one part in a few hundred: a process or material variation, such as a worn check ring, moisture or a cold nozzle.

Causes by source

Short shots are easier to solve when you sort the causes into four groups.

Part design

  • Long flow length through a thin wall. Many resins fill a flow length of roughly 100 to 200 times the wall thickness (typical, depends on the resin and the melt temperature). Beyond that, the melt freezes before it arrives.
  • Wall thickness steps. A thin section after a thick one fills last and may not fill at all.
  • Thin ribs and deep pockets. Narrow features act like small dead ends where air stays trapped.
  • No second gate where the part needs one. A large part sometimes needs two or more gates.

Mold

  • Gate too small or in the wrong place. The gate controls how much melt gets into the cavity and how long it stays open. A gate that freezes early stops the pack as well. See injection molding gate types.
  • Poor venting. Air must leave through the parting line, ejector pins or vent inserts. If a vent is blocked with residue, the air has nowhere to go and the melt stops.
  • Runner too long or too thin. A long, thin runner loses heat and pressure before the melt reaches the gate.
  • Unbalanced multi-cavity runner. One cavity fills first, another last. A mold flow study shows this. See mold flow analysis.
  • Cold slug or blocked nozzle. A frozen plug in the hot runner nozzle starves one drop.
  • Cooling too aggressive near the gate. A cold mold surface near a thin feature freezes the melt on contact.

Process

  • Shot size too small. The metering stroke does not deliver enough melt. Check the cushion, the small amount of melt left in front of the screw at the end of injection. A cushion near zero means the screw bottomed out and the shot is simply too small. A cushion that changes shot to shot points to a worn check ring.
  • Injection speed too low. The melt cools while it flows slowly. Thin walls often need fast fill.
  • Injection pressure or hold pressure too low. The machine cannot push the melt through the last part of the cavity.
  • Melt temperature too low. The resin is more viscous and freezes sooner.
  • Mold temperature too low. The frozen skin grows faster and narrows the flow channel.
  • Switchover too early. If the machine switches from speed control to pressure control before the cavity is nearly full, the last section fills slowly.

Material

  • Viscosity too high. A low melt flow grade fills thin sections badly. Switching to a higher flow grade of the same resin family often cures the problem, but only if the application allows it. Check heat resistance and impact strength first.
  • Moisture in a hygroscopic resin. Wet nylon, PC or PET can change viscosity and cause splay and short fills. See resin drying temperature chart.
  • Too much regrind. Ground runners and rejects change the viscosity and the feeding behavior.
  • Wrong lot or wrong grade. Confirm the resin lot and the grade on the process sheet.

Fixes in order of effect

Fix in this order: design, mold, process, material. The first two last for the life of the mold. The last two are quick but often only treat the symptom.

Step Typical action Who acts
1. Part design Thicken the thin section, add a second gate position, reduce flow length, round the thickness step Buyer with plant
2. Mold Enlarge the gate, add or clean vents, enlarge the runner, balance cavities, clear nozzle Plant tool room
3. Process Raise shot size, switchover and injection speed; raise melt and mold temperature within the resin window Plant process engineer
4. Material Move to a higher flow grade, dry the resin, cut the regrind ratio Buyer and plant jointly

A process fix that works only at the extreme edge of the window is not a fix. If the plant has to run the melt at the top of the resin’s temperature range and the pressure at the limit of the press, a small change of lot or weather brings the short shot back.

Need a quote for a molded part? Get matched with a molding plant

Quick checks at the press

A plant technician can narrow the cause in a few minutes.

  1. Weigh five shots. If the weights drift, check the check ring, the cushion and the feed.
  2. Run a short-shot series: increase the shot size in small steps and photograph each part. The fill pattern shows which feature fills last, which is where venting or a gate change helps.
  3. Check the vents on the last-fill area for residue.
  4. Check the hot runner nozzle temperatures and heater readings.
  5. Try a slightly higher mold temperature. If the problem disappears, the mold surface was freezing the melt.

What to ask the plant for

When you receive parts with a short shot or a warning from the plant, ask for:

  • Photos of the defective part next to a good one, with the location marked.
  • The process sheet before and after the fix: melt temperature, mold temperature, injection speed, switchover position, hold pressure and cushion.
  • The mold change record, if the gate or vents were modified.
  • Confirmation of the resin grade, the lot and the regrind percentage.
  • The root cause in one sentence, plus the action that prevents repeat.

If the fix was only a process change, ask what the margin is now: how far the machine sits from the limit in pressure, temperature and shot size. A formal 8D report may be needed for repeated defects. See 8D report for molded parts quality claims.

How to prevent short shots in a new program

Most short shots in production are decided in the first design review.

  • Share the wall thickness map early. Ask the plant to flag any flow length that looks long for the resin.
  • Agree the resin grade, including the melt flow range. A grade swap later changes the fill.
  • Ask for a fill simulation on large or thin parts.
  • Require a documented process window at T1. The plant should report the pressure and temperature range in which good parts are made, not only the setting it ended on.
  • Define the short shot as a reject in the inspection plan.

For the wider catalog of defects and where each comes from, read injection molding defects: causes and fixes. The opposite problem, excess plastic at the parting line, is covered in flash in injection molding.

Working with a rep

We are a manufacturers’ representative for injection molding plants. Buyers pay nothing for the introduction; the plant pays us a commission on orders from buyers we introduce. If your part is thin walled or has long flow paths, say so in the RFQ and we route it to the partner plant whose lane fits the resin and the press range. Send an RFQ with the drawing and your resin grade.

Frequently asked questions

Is a short shot the same as a burn mark or a sink mark?

No. A short shot is missing plastic: the cavity did not fill, so an edge, rib or corner is incomplete. A burn mark is a dark or brown area caused by trapped air heating under compression. A sink mark is a dimple caused by shrinkage over a thick section. A burn mark at the end of fill can sit next to a short shot, because both come from air that cannot leave the cavity.

Can a short shot be fixed by raising the injection pressure?

Sometimes, but it is the weakest fix. More pressure or speed fills the part, then often creates flash, high stress or burn marks. If the part only fills at the top of the machine's pressure range, the real cause is in the design, the gate or the vents, and the process has no margin left.

How many short shots are acceptable in a production lot?

None should reach the buyer. A short shot is a functional and visible defect, so the inspection plan should reject it by definition. Ask the plant how it detects short shots in production, for example by cushion monitoring, weight checks or visual inspection at the press.

Need a quote for a molded part?

Send the model. We match it to the partner plant whose lane fits and reply within 24 business hours. Free for buyers.

Get matched with a molding plant

Keep reading