Skip to content
Get matched

Guides / Quality

Sink marks in injection molded parts: causes by design, mold, process and material, and how to fix them

November 7, 2026

A sink mark is a small dip on the surface of a molded part, usually over a rib, boss or thick section. It happens because the plastic in the thick area shrinks as it cools and pulls the surface inward before the skin is rigid enough to resist. The fix is a thinner or better cooled thick section, a gate placed near it, and enough pack pressure and hold time to feed it until the gate freezes. Design fixes work best and process fixes work only to a point.

This post explains why sinks form, what each cause looks like and the order in which to fix them.

What a sink mark is and why it forms

When melt enters the cavity, it cools against the mold wall and forms a solid skin. The inside stays molten for longer. As the core cools it shrinks. If the gate is still open and pack pressure is on, more melt flows in to make up the volume. If the gate has frozen, or the pressure is too low, no more melt enters and the core pulls on the skin.

  • If the skin is soft, the surface is pulled inward and you see a sink mark.
  • If the skin is stiff, it holds its shape and the core tears away from itself, leaving a void.

Semi-crystalline resins such as PP, HDPE, PA and POM shrink more than amorphous ones such as ABS, PC and PS, so they show sinks more readily. Sink is worst where a thick section sits behind a visible face: under a rib, over a screw boss or at the junction of two walls.

How to recognize it

  • A shallow depression on the face opposite a rib, boss or thick area.
  • It shows more on glossy or dark surfaces because light reflects off the dip.
  • Texture hides it, a mirror polish shows it.
  • It can appear late: parts that look flat when ejected may show sink after hours of cooling.

Gauge the depth. A dip of 0.02 mm may be visible on a gloss black face and invisible on a grained one. State the limit and the face in your drawing.

Causes by category

Work through the categories in this order, because the earlier ones are more permanent and cheaper to fix on paper.

Part design

  • Thick sections. Any area much thicker than the nominal wall cools later and shrinks more.
  • Ribs too thick at the base. A rib at the same thickness as the wall leaves a thick spot at the junction. A typical base is about 50 to 60 percent of the wall for cosmetic parts. See rib design for molded parts.
  • Bosses attached to the wall. A boss with a thick wall of its own, or one joined to the face without ribs, is a common sink location. See boss design.
  • Wall thickness variation. Rapid changes in thickness leave pockets of heat. See wall thickness guidelines.
  • Intersections. Where ribs cross or a rib meets a boss, material builds up. Offset or core them.

Mold

  • Gate too small. A small gate freezes early and stops packing. A gate depth of about 50 to 75 percent of the wall is a common starting point for edge gates.
  • Gate far from the thick section. Pack pressure drops along the flow path. Put the gate in or near the thick area when possible. See gate types and gate location.
  • Runner too restrictive. A narrow runner or sprue loses pressure before it reaches the gate.
  • Uneven cooling. A hot spot behind a boss makes a local thick, hot zone. Cooling lines, baffles or bubblers in the core can fix it. See mold cooling design.
  • Poor venting. Trapped air resists packing in some designs.

Process

  • Pack pressure too low. The most common cause. Pack pressure should be high enough to feed the shrinkage without flash.
  • Hold time too short. If the gate has not frozen when pressure is released, melt flows back out of the cavity.
  • Melt temperature too high. Hotter melt shrinks more.
  • Mold temperature too high. The skin stays soft longer, and the core stays hot.
  • Cooling time too short. The part is ejected while the core is still hot and the skin is weak.
  • Cushion too small or zero. If the screw bottoms out, it cannot transmit pack pressure. A small stable cushion is needed.
  • Fill too fast or too slow. Both can lead to uneven packing.

Material

  • High shrink resin. Semi-crystalline resins, unfilled, shrink most.
  • Wrong grade. A grade with a lower melt flow or with nucleating agents may pack differently.
  • Moisture. Wet resin can cause splay, voids and inconsistent packing. See resin drying temperatures.
  • Fillers. Glass fiber reduces shrinkage and sink in many cases but increases warpage. Mineral filler reduces shrinkage too.
  • Blowing agents. Chemical foaming agents used on purpose in some parts offset sink. They change the surface and the strength.

Need a quote for a molded part? Get matched with a molding plant

Fixes in the right order

Fix design first, mold second, process third, material last. Process changes are quick but each has a limit and a cost.

Order Fix Notes
1 Core out thick areas from the back Best cure. Needs a mold change.
2 Reduce rib thickness at the base to about 50 to 60 percent of the wall Add draft and radius.
3 Move the gate nearer the thick area or enlarge it Mold change.
4 Improve cooling at the hot spot Mold change, cooling insert or bubbler.
5 Increase pack pressure and hold time Until the gate freezes. Check weight stability.
6 Reduce melt and mold temperature Within the resin window. Check fill.
7 Add texture on the cosmetic face Hides remaining dip. Needs extra draft.
8 Change the grade or add filler Check warpage, strength and cost.
9 Use gas assist or foaming on thick parts Process and cost change.

A gate freeze study helps with the process step. The plant molds at increasing hold times and weighs the parts. When the weight stops increasing, the gate is frozen. A hold time longer than that adds only cycle time.

What a good response from the plant sounds like

A plant that handles sink well can tell you:

  • Where the sink is and how deep, measured, with photos on the cosmetic face.
  • Which cause it suspects first and why.
  • What it changed in the process and the result.
  • Whether a mold change is needed, with a quote and a schedule.

Be careful with “we fixed it by raising pack pressure” when the increase also causes flash or stress. Ask to see the process sheet before and after.

What to ask for

When you find sink on a sample, send the plant:

  1. A photo with light raked across the face, and a scale or gauge.
  2. A drawing marking the face, the location and the limit you accept.
  3. A request for the process sheet and the change record: pack pressure, hold time, melt and mold temperature, cushion and cycle time.
  4. A weight check on a number of consecutive parts, to show the process is stable.
  5. A gate freeze study if the plant has not done one.

For parts that need to be approved, a limit sample helps both sides agree what is acceptable. See golden samples and limit samples. For a general chart of defects, see injection molding defects: causes and fixes.

Designing to avoid sink

Quick rules for designers:

  • Keep the wall uniform and core out thick sections.
  • Rib base at about 50 to 60 percent of the wall on cosmetic faces.
  • Add radius at rib bases, about 0.25 to 0.5 times the wall.
  • Bosses: connect with ribs or gussets instead of thickening the wall around them.
  • Use texture on large cosmetic faces.
  • Put the gate in the thickest section and flow thick to thin.
  • Tell the plant which faces are cosmetic at RFQ stage.

If you have a part with a sink problem and want a plant that runs similar parts, send an RFQ. We are a manufacturers’ representative: we route it to the partner plant whose lane fits, buyers pay nothing and the plant pays us a commission on orders from buyers we introduce.

Frequently asked questions

What is the difference between a sink mark and a void?

A sink mark is a dip on the surface. A void is a bubble-like hole inside the part. Both come from the same shrinkage in a thick section. If the skin is soft enough to be pulled inward, you get a sink. If the skin is rigid enough to stay put, the core pulls apart and leaves a void. Voids are harder to see, so a plant may need a cut section or X-ray to find them.

Can sink marks be fixed after the mold is made?

Often partly. Process changes such as more pack pressure or hold time, and gate changes in the mold, can reduce them. A fix to the part design, such as thinner ribs, usually needs a mold change, which costs more but works best. Surface texture on cosmetic faces can also hide sink at low cost.

Do sink marks matter on hidden faces?

Only if they affect fit, sealing or strength. Many drawings allow sink on non-cosmetic faces up to a stated depth. State that limit in the drawing so the plant does not spend time on a mark that does not matter.

Need a quote for a molded part?

Send the model. We match it to the partner plant whose lane fits and reply within 24 business hours. Free for buyers.

Get matched with a molding plant

Keep reading