Guides / Quality
Weld lines and knit lines in injection molding: causes, fixes and what to ask the plant
November 21, 2026
A weld line, also called a knit line, is a visible or structural seam where two flow fronts of molten plastic meet inside the mold and fail to blend fully. It shows as a thin line, a groove or a color streak, and it is usually weaker than the surrounding material. Weld lines come from the part shape, the gate layout, the mold temperature, injection speed and the resin, and they are fixed in that order: design first, then the mold, then the process, then the material. This guide explains the causes and gives the plant questions to ask.
What a weld line looks like
- A fine line, sometimes with a V-shaped groove on the surface.
- A color or gloss change along the line, common in metallic and pearlescent finishes.
- A crack or break along the line under load or after a drop.
- A visible line behind holes, around bosses or at the point where two gates meet.
Appearance and strength are separate problems. A weld line can look perfect and still be weak, or look poor and hold the load. Decide which matters for each part zone.
Why weld lines happen
Plastic enters the cavity at the gate and flows outward. When the front splits around an obstacle, such as a hole core, the two halves join on the other side. When two gates feed the same cavity, the fronts meet in the middle. Each front has cooled slightly on its way and carries a skin, so the surfaces do not mix as freely as they would in a single flow.
Fronts that meet head-on at a steep angle form a clear weld line. Fronts that meet at a shallow angle and flow together tend to merge better. Hotter melt, higher mold temperature and higher pressure at the meeting point help the fronts bond.
Short fibers make it worse. In glass filled resins, the fibers align along the flow direction and turn parallel to the line at the weld, so there is a resin-only bridge between the two sides. In such grades, weld strength can fall to a fraction of the strength elsewhere. In unfilled resins, the loss is often smaller but still present.
Root causes by category
Part design
- Holes, windows and bosses in the flow path, which force the melt to split.
- Sudden changes in wall thickness, which make flow race down the thick side and wrap around.
- Long flow length with thin walls, so the front cools before it meets.
- No clear location for the line, so it lands in a load path or on a cosmetic face.
Mold
- Gate position that places the weld line on a visible face or at a stress point.
- Several gates, or a hot runner with many drops, which create more meeting points.
- Poor venting at the weld location, so trapped air stops the fronts from joining and adds a burn mark.
- Gates that are too small, causing high shear and early cooling.
- Uneven cooling, which leaves cold spots near the line.
Process
- Melt temperature too low for the flow length.
- Mold temperature too low, which cools the fronts before they merge.
- Injection speed too slow, which lets fronts cool.
- Low packing pressure, which does not push the fronts together.
- Excessive moisture in the resin, which adds splay and weakens the bond.
Material
- High viscosity or low melt flow, which needs more heat and pressure.
- Glass fiber, mineral fillers and some pigments, which reduce bonding or make the line visible.
- Metallic flakes and pearl pigments, which line up along the weld and show a streak.
- Regrind with degraded material, which flows poorly.
- Masterbatch with poor dispersion, which shows a color line.
Fixes, in order
Work in this order. Design changes cost the least if made early, and process tweaks cost the least once the mold exists.
1. Change the design
- Move holes and bosses so the melt does not have to split across a large area, or ask whether they can be formed in a secondary operation.
- Make walls more even and add a flow leader, a slightly thicker channel that guides the melt to the far end.
- Give the part a location for the weld line, such as a thickened rib, and mark it on the drawing.
- Avoid placing load features, such as screw bosses and snap beams, on a weld line. See snap fit design.
2. Change the mold
- Move or add a gate so the weld lands on a non-critical area, and use mold flow results to guide it. See mold flow analysis and injection molding gate types.
- Use a larger gate to reduce shear and let more heat into the cavity.
- Add vents at the weld location, and an overflow well if needed, to carry cold material away from the line.
- Use sequential valve gating on large parts, so fronts meet in a controlled order. See hot runner vs cold runner.
- Raise local mold temperature with better cooling design. For cosmetic parts, rapid heat and cool systems raise the surface temperature during fill and are used to reduce visible lines.
3. Change the process
- Raise melt temperature in small steps, within the resin supplier’s limits.
- Raise mold temperature, especially near the weld.
- Increase injection speed, to deliver hotter melt to the weld.
- Raise holding pressure and time, to compress the line.
- Check drying and moisture.
- Change one setting at a time, and record it.
4. Change the material
- Choose a grade with higher melt flow.
- Use a lower fiber content, or a grade built for better weld strength where available.
- Pick a pigment or masterbatch known to disperse well, or reduce metallic flake.
- Cut or remove regrind.
A material change late in a program can be costly, so settle the choice before the mold is built, based on the load and cosmetic needs. For a related defect in the same family, see injection molding defects: causes and fixes.
Need a quote for a molded part? Get matched with a molding plant
Cosmetic and structural requirements
Write the requirement on the drawing. Examples:
- “No visible weld line in Zone A (marked).”
- “Weld lines allowed in Zone B, maximum visible length 10 mm, no groove.”
- “No weld line within 5 mm of the screw boss.”
The numbers above are examples; set your own from the part. For structural parts, specify the test. Strength tests cut samples across the weld, or load the finished part to a defined force, and compare to the value needed in use. For glass filled nylon, plan for a lower weld strength in design and keep the line out of the load path. See glass filled nylon injection molding.
What to ask the plant
When samples show weld lines, ask for:
- Photos of the line, with a scale and the lighting described.
- The mold flow report with weld line locations, if one exists, and a comparison with the real parts.
- The process sheet and the change record between the sample with the line and the improved one. See process change notification for molded parts.
- The melt and mold temperatures used, injection speed and hold pressure.
- A cross-section or strength test across the line.
- The list of options the plant considers, with their cost, such as moving a gate or adding a vent.
A good plant will tie the cause to one of the four categories and propose changes in the right order. If a plant proposes only to run hotter, ask what else it considered.
Weld lines in the RFQ
Put these in the RFQ so the plant can plan the gate position early:
- Cosmetic zones and the visibility requirement of each.
- Load paths and features that must not sit on a weld line.
- Resin and filler, so the plant knows how severe the issue is.
- Finish, since texture hides a line better than a high gloss.
Mention that you want a mold flow report with the weld lines shown, and a review of gate position at design review. See mold design review checklist.
Send a part with weld line limits
plasticmoldingfactories.com is a manufacturers’ representative for audited plastic injection molding plants. Buyers pay nothing; the plant pays us a commission on orders from buyers we introduce. Put the cosmetic zones and load paths in your RFQ, and we route it to the one partner plant whose lane fits, and you agree the gate layout with that plant directly.
Frequently asked questions
Are weld lines and knit lines the same thing?
The terms are used almost interchangeably. Some engineers reserve weld line for flow fronts meeting head-on, and meld line for fronts that meet at a shallow angle and merge more fully. Whichever words you use, state the location and the requirement on the drawing.
Can a weld line be removed completely?
Often not completely. If the part has a hole, boss or several gates, the melt must split and rejoin, so a weld line forms. You can move it, weaken its look, strengthen it or hide it with texture, but removing it needs a design change, such as a single gate and no obstructions.
How do I test whether a weld line is strong enough?
Use a test that loads the weld, such as a tensile or bend test on cut samples, a drop test on the finished part or a pressure or torque test for the function. Set the acceptance value from the real load, and compare parts with and without the weld.
Need a quote for a molded part?
Send the model. We match it to the partner plant whose lane fits and reply within 24 business hours. Free for buyers.
Get matched with a molding plant