Guides / Quality
Splay and silver streaks in injection molding: causes, fixes and what to ask the plant
November 21, 2026
Splay is a cosmetic defect that shows as silver or white streaks, usually fanning out from the gate in the direction of flow. The most common cause is moisture in the resin, which turns to steam in the barrel. Heat damage to the melt, trapped air and contamination come next. Check moisture and drying first, then melt temperature and residence time, then air and venting, then the mold and hot runner. Every step is cheap compared with scrapping a lot.
What splay looks like
Splay appears as streaks, often silvery, sometimes grey or white. They follow the flow path from the gate, and on a glossy or dark part they stand out. The streaks are tiny bubbles or gas pockets that were pulled across the surface by the flow front and burst on the mold wall, leaving a rough streak behind.
Splay is easy to confuse with other defects:
- Jetting is a snake-like pattern near the gate caused by melt spurting into the cavity before it fills, not a gas streak.
- Flow lines are wavy lines from slow flow or a cold mold, usually without silver color.
- Burn marks are dark or brown, from trapped air compressed and overheated.
- Delamination peels off in layers and points to a contaminated or incompatible resin.
If the streaks are silver, point back to the gate and change from shot to shot, the cause is likely gas. If they are in the same place on every shot, look for a mold surface problem.
Cause 1: moisture in the resin
Many resins absorb water from the air: nylon (PA), polycarbonate (PC), PET, PBT, ABS, PC/ABS, PMMA and TPU. When wet pellets melt at 220 to 300 degrees C, the water becomes steam. The steam either leaves silver streaks or, in condensation polymers such as PC, PET and nylon, breaks the polymer chains by hydrolysis. That second effect weakens the part. A splayed nylon or polycarbonate part can pass a visual check on a surface that is hidden and still be brittle.
Typical drying settings (always confirm against the resin supplier’s data sheet and the lot):
| Resin | Typical drying | Common target moisture before molding |
|---|---|---|
| ABS | 80 C, 2 to 4 hours | below about 0.1 percent |
| PC | 110 to 120 C, 3 to 4 hours | below about 0.02 percent |
| PA6 / PA66 | 80 C, 4 to 6 hours | below about 0.2 percent |
| PET | 140 to 160 C, 4 to 6 hours | below about 0.005 percent |
| PBT | 120 C, 3 to 4 hours | below about 0.03 percent |
| PMMA | 80 C, 3 to 4 hours | below about 0.05 percent |
Use these only as a starting reference. Our resin drying temperature chart goes deeper on time, dew point and hopper size.
Drying fails in these ways:
- A desiccant dryer with a dew point warmer than about minus 30 to minus 40 C.
- Hopper capacity smaller than the residence time needs at the actual throughput, so resin leaves the hopper before it is dry.
- Resin loaded cold into a hot hopper on a humid day, then dried again later. A bag left open on the floor does the same.
- A long, uninsulated hose that lets the hot dry resin cool and pick up moisture on the way to the press.
- Regrind that was not dried, or that was stored in an open bin.
Even polyolefins such as PP and PE, which are not hygroscopic, can cause moisture splay when pellets are cold and damp from condensation after being moved from a cold store into a humid shop. Let the bags reach room temperature before opening.
Cause 2: overheated or degraded melt
Melt that is too hot, or that sits too long in the barrel, breaks down and releases gas. Look for:
- Barrel or nozzle temperature set above the resin’s range.
- High screw speed or high back pressure that adds shear heat.
- Residence time longer than 5 to 10 minutes for heat-sensitive resins such as PVC, POM and PC. A shot size that uses only a small part of the barrel makes this worse.
- Hot runner zones set too high, or a dead spot where plastic sits and burns.
A common signal is splay that gets worse after a pause or a slow cycle. Purge the barrel and restart; if the first shots are clean and splay returns after a few minutes, look at the temperature and residence time.
Cause 3: trapped air
Air can enter the melt through the feed throat, or pull in when the screw decompresses (sucks back) too far. Air in the melt causes silver streaks that look like moisture splay but do not respond to drying.
- Reduce screw decompression after plasticizing.
- Check the check ring and barrel for wear, which lets melt flow backward and draws in air.
- Raise back pressure slightly to compress the melt and push air out.
- Check venting at the end of fill. Poor vents trap air that streaks when it is dragged along the surface.
Cause 4: volatiles and contamination
Some resins and masterbatches contain volatile additives, lubricants or low-molecular-weight fractions that vaporize in the barrel. Colorants carried in a wet or low-grade carrier can also add moisture. Contamination from a different resin, a purge compound that was not cleared or dirt in regrind can create streaks or layers.
Ask the plant to run a fresh sealed lot of virgin resin without colorant. If the splay disappears, the cause is in the colorant, regrind or earlier handling. Our post on masterbatch vs pre-colored resin explains how carriers behave.
Need a quote for a molded part? Get matched with a molding plant
Cause 5: mold and hot runner
- Condensation on a cold mold surface can print as a streak, especially in humid shops. Check that the mold is at working temperature before the first shots.
- A small coolant leak inside the mold can put water on the cavity surface. Pressure-test the cooling circuit if splay shows up in one cavity only.
- A hot runner nozzle with a damaged tip or a leak can add degraded plastic to the flow.
- A gate that is too small raises shear and local heat, which can create gas and streaks. Injection molding gate types covers sizing.
A simple diagnosis sequence
Splay causes overlap, so test in an order that rules out the easy ones first.
- Read the pattern. Same position every shot points to the mold. Random streaks from the gate point to material or melt.
- Check moisture. Use a moisture analyzer on a pellet sample taken from the hopper throat, not from the bag. Compare with the supplier’s limit.
- Do an air shot. Purge a shot of melt onto a clean surface. Foamy, bubbly or silver purge means moisture or degradation. A clear, smooth strand means the barrel is fine.
- Lower melt temperature by 10 to 20 C. If the splay fades, heat damage was part of it.
- Reduce decompression and screw speed. Check for air.
- Change one variable at a time. Write each change in the process record.
What the fixes look like in order
The fix order follows cost and risk:
- Part design. Rarely the cause, but very thick sections next to thin ones with a small gate can create high shear. Wall and gate guidance is in injection molding wall thickness.
- Mold. Repair or clean vents, fix leaks, resize gates or replace a worn hot runner tip.
- Process. Lower melt temperature, reduce residence time, adjust decompression and back pressure, and slow screw speed.
- Material. Dry correctly, replace the lot, change the colorant carrier or stop using regrind.
Start with material and process because they are the fastest and the cheapest to try, and then move to the mold only if the evidence points there.
What to ask the plant
If a lot arrives with splay, or an approval sample shows it, ask for:
- Close-up photos of the defect with the part orientation and gate position marked.
- The resin grade, lot number and drying record (temperature, time and dew point reading).
- A moisture reading taken at the hopper before the run.
- The process sheet with melt temperature, screw speed, back pressure and decompression, plus a note of any change made.
- The root cause and the corrective action in writing. Add a check of the parts made before and after the fix.
Plants that practice scientific molding, with a recorded process window, usually answer these quickly. For related reading, see scientific molding and the overview of injection molding defects, causes and fixes. For the resin behavior, the Wikipedia article on injection moulding gives neutral background.
Preventing splay on the next order
Put the defect into the purchase order as an acceptance criterion: state which faces are visible, what splay is rejected and what is allowed, and attach a reference photo. A plant that logs drying for each lot and holds a moisture limit per resin has a process that prevents it in the first place.
If you need a plant that already controls drying and process records for hygroscopic resins, send your part as an RFQ. We are a manufacturers’ representative and match each RFQ to the one partner plant whose lane fits the resin, press range and part type. You order from the plant directly, and it costs buyers nothing because the plant pays us a commission.
Frequently asked questions
Is splay only caused by wet resin?
No. Wet resin is the most common cause, but splay also comes from overheated or degraded melt, trapped air from screw decompression or a worn check ring, volatile additives in the resin, contamination and condensation on cold pellets. A purge test and a moisture reading help tell them apart.
Can parts with splay be shipped if the function is fine?
Only if the drawing or the approved sample allows it. Splay is a cosmetic defect on visible faces, but on a structural part it can mark a weakened material, because the same moisture that causes splay can break down nylon, PET and polycarbonate chains. Ask the plant to confirm the cause before you accept a lot.
Does a dryer on the machine guarantee dry resin?
No. The dryer needs the right temperature, time and dew point, a sealed hose to the hopper and a correct hopper size for the throughput. A dryer that is too small, a clogged filter or a wet return air line can leave resin as damp as it was before drying.
Need a quote for a molded part?
Send the model. We match it to the partner plant whose lane fits and reply within 24 business hours. Free for buyers.
Get matched with a molding plant