Guides / Materials
Polycarbonate injection molding: drying, molded-in stress and keeping parts clear
November 21, 2026
Polycarbonate (PC) is molded dry, hot and with low stress, and those three words explain most of what goes right or wrong with it. Dry the resin until moisture is far below what other plastics tolerate, run the melt at about 280 to 320 degrees C and keep the mold warm. Then design the part with generous radii and even walls, because PC is tough in a smooth part and brittle at a sharp corner. Get these wrong and you see splay, bubbles, haze, yellowing or cracks that appear after the part is shipped.
PC is used where you need clarity, impact strength and heat resistance together: lenses, covers, light guides, housings, safety parts and electrical components. It costs more than ABS and is harder to mold well. This post covers the settings that matter, the defects to watch and what to ask a plant.
Typical processing window
These are typical ranges for general-purpose grades. The resin datasheet and the plant’s own trials decide the actual settings. Do not treat the numbers as a guarantee.
| Parameter | Typical range |
|---|---|
| Drying temperature | 110 to 120 degrees C |
| Drying time | 3 to 4 hours |
| Moisture before molding | Below about 0.02 percent (some optical uses ask for less) |
| Melt temperature | 280 to 320 degrees C |
| Mold temperature | 80 to 120 degrees C |
| Mold shrinkage | About 0.5 to 0.7 percent |
| Typical wall thickness | 1 to 4 mm |
For other resins and their dryer settings, see resin drying temperature chart.
Drying: the step that cannot be skipped
PC absorbs moisture from the air. At melt temperature, water reacts with the polymer chain in a process called hydrolysis and cuts it into shorter chains. The part may look fine yet be weaker. In the worse case you see silver streaks, bubbles or a cloudy surface.
Good drying practice:
- Use a desiccant (dehumidifying) dryer, not a plain hot-air oven, with a dew point of about minus 40 degrees C or lower.
- Dry for the time on the datasheet, and do not shorten it because the hopper looks dry.
- Keep the dried resin dry. Resin left in an open hopper over a break can re-absorb moisture. Hopper lids and short transfer lines help.
- Check moisture with a moisture analyzer if the part is critical. Ask the plant if it does this.
- Dry regrind too. It has been exposed to air and heat.
Ask the plant for its dryer type, drying time and dew point for the job. Silver streaks on a PC part usually point first at drying. See splay in injection molding for the full list of causes.
Melt temperature and residence time
PC needs a high melt temperature to flow, but it is sensitive to heat over time. If melt sits in the barrel too long, it yellows and loses toughness. Two practical points:
- Match shot size to barrel size. A shot that is very small compared with the barrel means long residence time. A common rule is to use roughly 20 to 80 percent of the barrel capacity, with the plant’s experience deciding.
- Avoid dead spots in hot runners. Material that stagnates in a hot runner turns brown and sheds black specks into the parts.
At shutdown, a plant should purge PC out of the barrel and not leave it sitting hot.
Molded-in stress and stress cracking
Molded-in stress is frozen-in strain left when the melt cools under pressure. In PC it comes from:
- Fast injection into a cold mold. The skin freezes in tension.
- Overpacking near the gate. Too much pressure or hold time.
- Small gates. High shear at the gate leaves stress there.
- Sharp corners and sudden thickness changes.
- Ejection forces from too little draft or a rough surface.
Stressed PC is vulnerable to environmental stress cracking. Common triggers are solvent cleaners, some adhesives and paints, oils and greases and certain plasticizers in nearby soft parts. Cracks often start at a gate, a weld line or the base of a screw boss.
On clear PC parts, you can see stress in polarized light as colored fringes. It is a quick check for the plant to run on first samples and for you to ask for in a T1 report. See first article inspection for plastic parts.
Design rules that lower stress
- Corner radius of at least about half the nominal wall thickness on inside corners. A sharp inside corner is where PC parts break.
- Even wall thickness, with gradual changes. See injection molding wall thickness.
- Draft of at least 1 degree on most faces, more for textured or deep parts. See draft angle in injection molding.
- Bosses with ribs and radii at the base, and screw hole sizes matched to the thread-forming screw the assembly needs.
- Gates placed away from areas that carry load or meet chemicals, and large enough to avoid high shear.
Need a quote for a molded part? Get matched with a molding plant
Clarity and appearance
If the part must be clear, every contamination and surface defect shows.
- Black specks come from burned resin in the barrel or hot runner, or from dirt in the resin. Ask about screen, purge and cleaning practice.
- Haze often comes from moisture, contamination with another polymer or an overly cold mold surface.
- Yellow tint comes from heat damage or long residence time, and from some stabilizer packages.
- Flow lines and weld lines are more visible in clear PC. Place gates so the weld lines fall outside the viewing area when you can. See weld lines in injection molding.
- Mold surface must be polished to match. High-polish optical parts typically need a high SPI polish on the cavity and good venting, and the mold steel must be a grade that takes a polish.
Never mix PC with other resins in the same hopper or barrel without a purge. Acetal (POM) in particular reacts badly with PC at melt temperature and can ruin both the parts and the screw.
Grades and blends
PC comes in many grades, and the right one depends on the use.
- General purpose, with different melt flow rates. A higher melt flow fills thin walls more easily but gives up some toughness.
- Flame-retardant, often required for electrical housings. See UL94 V-0 plastic for what the rating means.
- UV-stabilized for outdoor light. Compare options in UV-resistant plastic.
- Glass-filled, for stiffness and lower shrinkage, but with less clarity and higher wear on tooling.
- PC/ABS blends, which are easier to mold and cheaper, with some loss in clarity and heat resistance. See ABS vs PC/ABS.
Name the exact grade in your RFQ, or ask the plant to quote a named grade and state the alternatives it would accept. “Polycarbonate” alone leaves too much open.
What to put in the RFQ
- Resin grade, color and any flame, UV or food-contact requirement.
- Whether regrind is allowed, and if so the maximum share.
- Clarity and cosmetic requirements: allowed black specks, flow lines and gate vestige, with a limit sample if you have one.
- Chemicals the part will meet in use, such as cleaners or adhesives.
- Stress or drop test requirements.
- Required drying records and resin lot traceability. See resin lot traceability records.
What a good answer from a plant sounds like
A plant with PC experience will name its dryer type and dew point, ask which grade you want, ask about the chemicals the part will meet and propose a gate location with a reason. It will also tell you if your corner radii are too small. If the reply is only a price, ask the questions above before you send a PO.
When your part and grade are clear, send the package as an RFQ. We are a manufacturers’ representative: we match the package to a partner plant whose lane fits the resin, press range and part type. It costs buyers nothing. The plant pays us a commission on orders from buyers we introduce, and you order directly from the plant.
Frequently asked questions
Can I reuse regrind in polycarbonate parts?
For general grades, plants often allow a limited share of clean, dried regrind, commonly in the range of 10 to 25 percent. For optical, clear or flame-rated parts, many buyers allow none. Decide this in the RFQ, because regrind lowers impact strength a little each time it is processed.
Why do polycarbonate parts crack weeks after molding?
Usually molded-in stress combined with a chemical. Cleaners, adhesives, oils and some plasticizers attack stressed polycarbonate and cause cracks that start at gates, sharp corners and screw bosses. Lower stress in the mold and process, add radii and test the part with the real chemicals it will meet.
Is polycarbonate suitable for outdoor use?
Plain polycarbonate yellows and loses surface quality in sunlight. UV-stabilized grades or a coating are used outdoors. Check the grade datasheet and the weathering data for your exposure before you choose.
Need a quote for a molded part?
Send the model. We match it to the partner plant whose lane fits and reply within 24 business hours. Free for buyers.
Get matched with a molding plant