ABS vs PC/ABS for molded enclosures: heat, impact, flame rating, cost and processing
November 5, 2026
Specify ABS when the enclosure needs good looks, easy molding and low material cost at normal indoor temperatures. Specify PC/ABS when it needs higher heat resistance, better impact strength, especially in the cold, or a flame retardant grade for electronics. PC/ABS usually costs more per kilogram and molds at higher temperatures, but it is a common step up from ABS for housings that get warm, get dropped or must meet a flammability rating.
This post compares the two on the properties that decide an enclosure, and lists what to put in the RFQ.
What each material is
ABS (acrylonitrile butadiene styrene) is an amorphous thermoplastic made of three monomers. Acrylonitrile adds chemical resistance and heat resistance, butadiene adds toughness and styrene adds gloss and ease of flow. It is one of the most widely used resins for housings, appliance parts and consumer products. The Wikipedia page on ABS is a neutral overview.
PC/ABS is a blend of polycarbonate and ABS. The PC adds heat resistance and impact strength. The ABS keeps the melt easier to process and cuts cost compared with straight PC. The ratio varies by grade, so two PC/ABS grades from different suppliers can behave quite differently.
Both are amorphous, so they shrink less than semi-crystalline resins and hold dimensions fairly well.
Property comparison
Values are typical for general-purpose unfilled grades. Grades vary, so use the supplier datasheet for design.
| Property | ABS (typical) | PC/ABS (typical) |
|---|---|---|
| Heat deflection temperature, 1.8 MPa | about 80 to 100 C | about 95 to 120 C |
| Notched Izod impact | moderate to high | high, holds better at low temperature |
| Stiffness | moderate | similar to somewhat higher |
| Flow in molding | very good | good, a little stiffer |
| Mold shrinkage | about 0.4 to 0.7 percent | about 0.5 to 0.7 percent |
| Surface finish | excellent gloss or texture | excellent, textures well |
| Price per kg | lower | higher, commonly by tens of percent |
| Flame retardant grades | available | widely available |
| Chemical resistance | good against many cleaners, weak against some solvents | similar, with stress cracking risk from some chemicals |
| Plating | common substrate for decorative plating | plating grades exist |
Treat the heat figures as a guide to relative rank. For a real design, check the continuous use temperature, the UL relative thermal index if it applies and the heat deflection at the load your part sees.
Heat
ABS softens around 100 C at the glass transition, and it creeps under load well before that. An enclosure that sits next to a power supply, a motor or in a hot vehicle cabin may warp in ABS and hold in PC/ABS.
Common cases:
- Indoor consumer products at room temperature: ABS is usually enough.
- Electronics with internal heat sources: PC/ABS gives more margin.
- Parts left in a parked car or in sun: surface temperatures can exceed 70 C, so check both heat and UV.
- Parts through a hot wash or sterilization: neither is a high-temperature resin, so look at the specific cycle.
Impact and low temperature
PC/ABS holds its toughness at low temperature better than ABS. If the product is dropped, used outdoors in winter or shipped through cold climates, PC/ABS is the safer choice. ABS also impacts well at room temperature, but it becomes more brittle in the cold.
Impact performance also depends on part design. Sharp inside corners, thin ribs and weld lines are weak points in either resin, and a radius on every inside corner often matters more than the resin change. See wall thickness guidelines for the rules on corners and transitions.
Flame retardancy
Many electrical enclosures need a UL94 flame rating, often V-0 or V-1, at the part’s thickness. Both resins come in flame retardant grades, but PC/ABS is the more common base for V-0 grades in thin walls. Rules to follow:
- The rating belongs to a grade, in a color, at a stated thickness. A V-0 at 1.5 mm does not apply to a 1.0 mm wall.
- Changing color or masterbatch can break the rating. Use the color the grade was listed with, or a listed color option.
- Regrind can lower the rating or shift it. Check the allowed percentage.
- Ask for the UL yellow card for the grade and keep it in the file.
Check the current text of the standard and the UL listing for your grade. The ul.com site is the neutral source, and the topic is covered further in UL94 V-0 resins for electrical enclosures.
Halogen-free flame retardant grades exist for both. If your customer or region restricts halogens, say so in the RFQ.
Cost
PC/ABS usually costs more per kilogram than ABS, often by tens of percent, and flame retardant grades cost more than standard ones. Prices move with oil, feedstock and region, so ask each plant to quote the exact grade with the resin cost shown.
Part cost also includes processing. PC/ABS needs a higher melt temperature, more drying and often a hotter mold, so cycle time may be a little longer. Weigh the added cost against what you save in rejects, warranty returns or redesign.
If the resin price may swing, see resin surcharge clauses for how to handle it in the contract.
Need a quote for a molded part? Get matched with a molding plant
Molding differences the plant manages
| Item | ABS (typical) | PC/ABS (typical) |
|---|---|---|
| Drying | about 80 C for 2 to 4 hours | about 90 to 100 C for 3 to 4 hours |
| Melt temperature | about 210 to 250 C | about 240 to 270 C |
| Mold temperature | about 50 to 80 C | about 60 to 90 C |
| Moisture risk | moderate | high, causes splay and brittleness |
These are typical windows, and the grade datasheet governs. Two points matter to the buyer:
- Drying. Both absorb moisture. Wet PC/ABS can show splay and lose impact strength, because the polycarbonate in the blend can break down in the presence of moisture at melt temperature. Ask whether the plant dries resin in a desiccant dryer and logs the dryer settings. See splay and silver streaks.
- Residence time. PC/ABS can degrade if left in the barrel too long. A plant running a small part on a large press may have this problem.
Weld lines, sink and warpage appear in both. PC/ABS has a visible weld line on some textured or dark surfaces, so put the gate where the weld falls on a hidden face.
Finishes: paint, texture, plating
- Texture: both take texture well. Higher textures need more draft. See mold texture standards.
- Paint: both can be painted, but paint can attack stressed PC blends, so stress and solvent must be tested together.
- Plating: ABS is the classic plating substrate. PC/ABS plating grades are used on automotive trim.
- Ultrasonic welding and gluing: both weld well. Select adhesives and solvents carefully for PC/ABS because of stress cracking.
- UV: neither is UV stable in standard grades. Outdoor parts need a UV-stabilized grade or a coating.
How to decide
Use this list in order:
- Does the part need a flame rating? If yes, look at PC/ABS flame retardant grades first.
- What is the highest temperature the part sees in use and in shipping? If it exceeds about 70 to 80 C, ABS is marginal.
- Will it be dropped, or used in the cold? Choose PC/ABS.
- Is it purely cosmetic, indoors, at room temperature? ABS is likely enough and costs less.
- Does it need plating? Start with an ABS plating grade or a certified PC/ABS plating grade.
- Will the plant be running it on a mold made for ABS? Check gate size, venting and cooling.
What to put in the RFQ
State the resin by grade or an approved list, not only by family. Include the color, the flame rating and minimum wall it applies to, the finish and any regulatory need such as RoHS. Give the highest service temperature and the test or standard you use. Ask each plant to name the resin supplier and grade it plans to use. For other materials see polycarbonate molding: drying, stress and clarity.
When the specification is ready, send an RFQ. We are a manufacturers’ representative: we match it to the partner plant whose lane covers the press range and resin, you order from that plant directly and it costs buyers nothing, since the plant pays us a commission on orders from buyers we introduce.
Frequently asked questions
Can I replace ABS with PC/ABS without changing the mold?
Often yes, because the shrink rates are close, but you must confirm with the plant and the resin datasheet. PC/ABS is stiffer to fill and needs a higher melt temperature, so gates, venting and cooling may need adjustment. Run a trial and re-measure critical dimensions before you release the change.
Is PC/ABS good for painting and plating?
Yes for painting, with grades and paint systems that suit it. Plating grades exist for both ABS and PC/ABS, and ABS is the more common substrate for decorative plating. If your part needs plating or a specific paint, name the finisher and test a sample early.
Do ABS and PC/ABS both come in UL94 V-0?
Both exist in flame retardant grades, and PC/ABS is the more common choice for V-0 enclosures. A rating applies to a grade at a stated thickness and color, not to the resin family. Ask the plant for the UL yellow card for the exact grade, color and minimum wall you will use.
Need a quote for a molded part?
Send the model. We match it to the partner plant whose lane fits and reply within 24 business hours. Free for buyers.
Get matched with a molding plant