Guides / Tooling
Multi-cavity mold balance: why cavities differ and how to prove they match
November 21, 2026
A multi-cavity mold is balanced when every cavity fills at the same time, with the same pressure and temperature, so every cavity makes the same part. Perfect balance does not exist, so the working question is how much difference you accept and how you prove it. Check three things before you approve a multi-cavity mold: a fill balance test, a per-cavity dimension report and a per-cavity process record. This article explains why cavities differ and what to ask the plant.
Why cavity balance matters
In a 4, 8 or 16 cavity mold, parts from different cavities can differ in weight, dimensions, gloss and strength. If one cavity runs at 98% of the weight of the others, it is probably under-packed and may have more sink or lower density. If one fills first, it may flash while the last one is still short.
The effects show up as:
- Out-of-tolerance dimensions in one cavity while the others pass.
- Cosmetic defects concentrated in one cavity, such as sink, weld lines or splay.
- Unstable process. The process window narrows, because a setting that suits one cavity pushes another into flash or short shot.
- Scrap and sorting cost. A cavity that cannot hold tolerance must be blocked off or sorted, which cuts output.
The value of a multi-cavity mold comes from output per cycle. Cavity variation takes some of that value back (see how many cavities an injection mold needs).
Natural balance and artificial balance
Runner layouts fall into two types.
- Naturally balanced. Every cavity sits at the same flow path length from the sprue, with the same number of turns and splits. Typical layouts are an H pattern for 4 and 8 cavities, or a radial layout. The melt travels the same distance to each cavity.
- Artificially balanced. Cavities sit at different distances, and the runner and gate sizes are changed so that all cavities fill at the same time. Common in layouts with a straight line of cavities or with family molds.
Natural balance is the starting point where the part and layout allow it. Artificial balance needs flow simulation and tuning during trials (see mold flow analysis).
Balance in the geometric sense is necessary but not enough, as the next section shows.
Shear imbalance: balanced geometry, unbalanced melt
Even in a naturally balanced runner, the cavities often do not fill the same. As melt flows through a cold runner, the layer near the wall is sheared, heats up and flows differently from the core. At each split, the sheared layer ends up on one side. The branch that receives more of the hot, thinner layer fills faster than the other.
The result is a repeated pattern: the inner cavities fill first, or one side of the mold is favored. It can occur in cold runners and in hot runner manifolds. Plants address it by:
- Changing gate or runner sizes by a small amount, based on short shot results.
- Using melt rotation or turning the runner designs that remix the layers before each split.
- Adjusting hot runner nozzle temperatures per drop.
These fixes belong in the design review for molds with many cavities or tight tolerances. For runner type tradeoffs, see hot runner vs cold runner.
Other causes of cavity variation
Runner shear is the best known cause, but not the only one.
| Area | Cause | Effect |
|---|---|---|
| Cavity steel | Small differences in cavity dimensions from machining | Dimension offset in one cavity |
| Cooling | Uneven flow or temperature between cavities | Different shrinkage and warp |
| Venting | A cavity that vents less traps gas | Short shot, burn marks |
| Gate | Differences in gate size or wear | Fill and pack differences |
| Hot runner | Nozzle temperature difference | Color, flow and sink differences |
| Mold wear | Wear or damage in one cavity | Flash or dimension drift |
Because many causes combine, measuring each cavity is the only reliable method.
How to test balance: short shot study
A short shot study is the standard fill balance test. It is simple and cheap.
- Run the mold at normal settings and reduce shot size until parts are incomplete, typically in steps from about 50% to 95% of full fill.
- Photograph or weigh the short parts from each cavity at each step.
- Compare how far each cavity has filled at the same moment.
- A balanced mold fills all cavities to the same level. An unbalanced mold shows one cavity ahead.
The result is a picture the plant can add to the T1 report. If the imbalance is large, fix the mold. If it is small, document it.
For a fuller trial sequence, see T1, T2 and T3 mold trials.
Need a quote for a molded part? Get matched with a molding plant
How to test balance: weight and dimensions per cavity
Weigh and measure parts by cavity, not by the batch.
- Weight. Weigh a set of parts from each cavity on a scale with enough resolution. Calculate the average and the spread between cavities. Any cavity far from the group points to a gate, venting or cooling issue.
- Dimensions. Measure the critical dimensions on parts from every cavity and show the results by cavity. A pooled average hides the problem; a chart by cavity shows it.
- Capability. Calculate Cpk by cavity as well as for the mold (see Cpk in injection molding). A mold with an acceptable overall Cpk can still hide one cavity with a poor value.
Numbers like a weight spread of about one percent are typical targets for many parts, not rules. A part with tight dimensions or a precision fit needs a tighter spread.
Mark cavities on the part
To measure by cavity, the part needs a cavity number. Most molds carry a small numbered insert in each cavity so every part shows where it came from. Specify where on the part the number goes: a hidden or non-cosmetic area, not a datum or functional surface. This also helps with traceability (see resin lot traceability records).
Without a cavity number, a defect in the field cannot be tied to a cavity, and you cannot find which cavity to repair.
What to ask the plant
- Is the runner layout naturally or artificially balanced, and was it simulated?
- Can you show the short shot study photos or weights per cavity?
- Will the T1 report list dimensions for every cavity?
- Are cavities numbered on the part and where?
- How will cavity data be tracked in production, and at what interval?
- What is your rule when one cavity drifts: block it, repair it or sort?
- If a cavity is blocked off, will you tell me first and agree on the rate and delivery effect?
Blocking a cavity is a common fix, but it changes output per hour and the piece price. A good plant tells you before it happens.
During production
A mold balanced at T1 can drift. Track these signs:
- Weight by cavity at start-up and at set intervals.
- Dimensions by cavity at set intervals on critical features.
- Process changes. Any change in melt temperature, injection speed or hold pressure can shift balance.
- Mold maintenance. After cleaning or repair, check balance again (see injection mold maintenance cost).
If you plan to move the mold to another plant, ask for the balance data and the process sheet. They shorten requalification.
When fewer cavities are the answer
If you cannot get acceptable balance, or the part is tight in tolerance or highly cosmetic, fewer cavities may give lower total cost. A 2-cavity mold that holds tolerance in both cavities is better than an 8-cavity mold that needs sorting. Volume, tolerance and cost per part together decide. For family molds that make several parts at once, balance is harder still (see family molds in injection molding).
Next step
Put cavity-level data in your RFQ and quality agreement: weight spread, per-cavity dimensions at T1 and cavity numbering. If you want those requirements quoted by a plant that works this way, send an RFQ. We are a manufacturers’ representative for audited plastic injection molding plants. We match your request to the one partner plant whose lane fits the part. Buyers pay us nothing, and the plant pays us a commission on orders from buyers we introduce.
Frequently asked questions
How much cavity-to-cavity variation is acceptable?
It depends on part size, tolerance and resin. For many parts the weight spread between cavities is held to around one percent or less, and dimensions must all sit inside the drawing tolerance with capability data per cavity. Agree the limit with the plant before the mold is built.
Can a plant fix an unbalanced mold by process settings alone?
Only partly. Changing temperature or injection speed can shift the balance, but a fix that depends on a narrow process window is fragile. A permanent fix, such as changing gate size or runner geometry, is more stable and should be done in the mold.
Why do outer cavities fill late?
In many runner layouts, melt near the runner wall is slower and cooler than melt in the core. When the runner splits, one branch gets more of the hot core melt than the other. That shear effect shifts fill and quality toward the favored cavities, even when the runner looks symmetric.
Need a quote for a molded part?
Send the model. We match it to the partner plant whose lane fits and reply within 24 business hours. Free for buyers.
Get matched with a molding plant